Glaze adhesive formula

formula
Component dosage /g component dosage /g
Glass Enamel Powder 50 Sodium Silicate
Iron Oxide 50   
Preparation and curing     The glass glaze and iron oxide were passed through a 320 mesh sieve, weighed and transferred to a paste with sodium silicate.
First cure at room temperature for 3 hours , then cure at 40 to 60 degrees for 3 hours , cure at 80 to 100 degrees for 3 hours , and cure at 120 to 150 degrees for 2 hours .
use   The glue is used for bonding of metal and ceramic parts, and the heat-resistant temperature is 400 °C.